Objective Brazing carbide teeth to a steel jaw in less than 5 minutes
  Material Steel pipe jaw, 0.5” (12.7mm) dia, 1.25” (31.75mm) long, 0.25” (6.35mm) thick carbide teeth, black flux and silver copper braze shims
  Temperature 1292ºF (700ºC)
  Frequency 257kHz
  Equipment • Power of 6 kW induction heating system, equipped with a remote workhead containing one 0.66μF capacitor
  • An induction heating coil designed and developed specifically for this application.
  Process A two turn rectangular helical coil is used to heat the carbide and steel to 1292ºF (700ºC) for 4 to 5 minutes. Three braze shims control the amount of braze and the even heat allows for a good flow of braze creating an aesthetically pleasing bond.
  Results/Benefits Induction heating provides:
  • Hands-free heating that involves no operator skill for manufacturing
  • Consistent, repeatable aesthetically pleasing brazes
  • Even distribution of heating  
   
  Brazing carbide teeth to steel pipe  